Sunday, January 3, 2010

Weld Lines

Weld Lines

Description

Weld Lines are created when two or more melt flow fronts meet possibly causing a cosmetically visible line. It can also create a weakened area in the finished molded part especially with filled resins.

Possible Solutions

  • Increase injection pressure.
  • Increase injection speed.
  • Increase injection hold.
  • Increase melt temperature.
  • Increase mold temperature.
  • Make sure part contains no sharp variation in cross-sections.
  • Vent cavity in the weld area.

Warping, Part Distortion

Warping, Part Distortion

Description

Warping, Part Distortion is shows up as parts being bowed, warped, bent or twisted beyond the normal specification outlined on the drawing.

Possible Solutions

  • Adjust melt Temperature (increase to relieve molded-in stress, decrease to avoid overpacking). stress, decrease to avoid over packing). stress, decrease to avoid over packing).
  • Check gates for proper location and adequate size.
  • Check mold knockout mechanism for proper design and operation.
  • Equalize/balance mold temperature of both halves.
  • Increase injection-hold.
  • Increase mold cooling time.
  • Relocate gates on or as near as possible to thick sections.
  • Try increasing or decreasing injection pressure.

Voids

Voids

Description

Voids are hollows created in the part. They are normally found in thick sectioned parts caused by material being pulled away from the hot center section towards cold mold walls leaving a void in the center.

Possible Solutions

  • Clean vents.
  • Decrease injection speed.
  • Decrease melt temperature.
  • Dry material.
  • Increase injection pressure.
  • Increase injection-hold.
  • Increase mold temperature.
  • Increase shot length.
  • Increase size of gate.
  • Increase size of sprue and/or runners and/or gates.

Valve Pin Does Not Close

Valve Pin Does Not Close

Description

Valve pin does not close properly. This will leave the gate protruding from the part. This may also occur if the valve pin is too hot, the material may stick to the valve pin.

Possible Solutions

  • Valve pin is too short. Check and replace if necessary.
  • Valve pin fit. Ensure that the valve pin is lapped to the gate steel when appropriate.
  • Damaged gate. Check if valve pin is too long, rework if necessary. Also check to ensure that the valve pin is concentric with the gate, if not replace it.
  • Hydraulic / Pneumatic seals may be worn. Replace as necessary.
  • Insufficient pin/land area in the gate area of the mold. Increase the gate area cooling, or increase the valve pin land contact.
  • Insufficient hydraulic or air pressure. Increase the pressure up to but not beyond the maximum rating of the unit being used.
  • Excessive hold time. Decrease the hold time.

Undersized Part

Undersized Part

Description

Part is too small when compared to the drawing specifications.

Possible Solutions

  • Decrease mold temperature.
  • Increase booster time.
  • Increase cylinder temperature.
  • Increase hold-time.
  • Increase holding pressure.
  • Increase injection pressure.
  • Increase injection speed.
  • Inspect mold for surface defects.

Surface Finish (Scars, Wrinkles)

Surface Finish (Scars, Wrinkles)

Description

Surface Finish (Scars, Wrinkles). Is the appearance of the ripples or wrinkles on the surface of the molded part.

Possible Solutions

  • Decrease back pressure.
  • Decrease nozzle temperature.
  • Increase booster time.
  • Increase the melt temperature.
  • Increase injection pressure.
  • Increase injection speed.
  • Increase overall cycle time.
  • Increase shot size.
  • Inspect mold for surface defects.

Surface Finish (Low Gloss)

Surface Finish (Low Gloss)

Description

Surface Finish (Low Gloss). Gloss is the appearance of the surface of the molded part when light is reflected off of it. Molds that are textured or resins that are filled have an inherently reduced level of gloss when compared to highly polished mold surfaces.

Possible Solutions

  • Clean mold surface.
  • If the part design allows increase the polish of the molding surface.
  • Increase cylinder temperature. This applies to molds that have a polished surface.
  • Increase injection pressure. This applies to molds that have a polished surface.
  • Increase injection speed. This applies to molds that have a polished surface.
  • Increase mold temperature. This applies to molds that have a polished surface.
  • Decrease cylinder temperature. This applies to molds that have a textured surface.
  • Decrease injection pressure. This applies to molds that have a textured surface.
  • Decrease injection speed. This applies to molds that have a textured surface.
  • Decrease mold temperature. This applies to molds that have a textured surface.
  • Increase melt temperature.
  • Make sure venting is adequate.