Sunday, January 3, 2010

Splay Marks, Silver Streaks

Splay Marks, Silver Streaks

Description

Splay Marks, Silver Streaks are usually caused by water vapor blisters at the flow front burst and freeze on the wall of the molding surface.

Possible Solutions

  • Check for contamination.
  • Decrease melt temperature.
  • Decrease nozzle temperature.
  • Dry resin pellets before use. As per the manufacturers recommendations.
  • Incorrect storage of pellets. Moisture on the pellets could be transferred into the melt, especially if the resin is not normally pre-dried.
  • Raise mold temperature. This will prevent condensation on the mold walls from being carried into the melt.
  • Ensure the mold is not leaking water onto the cores or cavities. Again this will prevent condensation on the mold walls from being carried into the melt.
  • Relocate gates on or as near as possible to thick sections.
  • Shorten overall cycle.

No comments:

Post a Comment